Lightweight floor and ceiling screeds, known as perlite concrete, using PERLITE EP 150 or EP 180 have the following properties:
- bulk density: 300–1000 kg/m3,
- thermal conductivity: 0.0065–0.23 W/(m x K),
- fire resistance: up to 900°C,
- compressive strength: from 0.5 to 6 MPa.
Perlite concrete is one of the best building materials used for the thermal insulation of floors, ceilings, and flat roofs. Perlite concrete screeds (with a thickness of 3 to 15 cm, depending on requirements) feature excellent insulation properties, sound absorption, fire resistance, lightweight nature, and are completely safe for health.
Preparation instructions for perlite concrete
Perlite concrete is prepared in the same way as standard concrete, except that PERLITE EP 150 or PERLITE EP 180 is used instead of sand. Depending on the perlite-to-cement ratio, mixes with compressive strength ranging from 0.5 to 6.0 MPa and thermal conductivity from 0.06 to 0.24 W/(m x K) can be achieved.
Formulas and physicochemical data of typical perlite concrete mixes
| PTB Designation | 300 | 400 | 500 | 600 | 700 | 800 | 900 | |
| Perlite EP 180 (1 bag) | m3 | 0.125 |
0.125 |
0.125 |
0.125 |
0.125 |
0.125 |
0.125 |
| Cement | kg | 12 | 19 | 27 | 35 | 42 | 42 | 50 |
| Water | l | 65 | 60 | 42 | 39 | 35 | 35 | 37 |
| Bulk density | kg/m3 | 300 | 400 | 500 | 600 | 850 | 1000 | 1000 |
| Thermal conductivity | W/mK | 0.065 | 0.078 | 0.092 | 0.100 | 0.120 | ||
| Compressive strength | MPa | 0.50 | 0.70 | 1.80 | 3.00 | 4.00 | 5.00 | 6.00 |
In order to improve the workability and plasticity of the mixes, a plasticizer can be added.
The individual components should be added in the following order: water – plasticizer – cement – perlite; mixing time is max. 6 minutes.